AA-Standards Klasse 5454 O
Eigenschaften
Allgemeines
Eigenschaft | Wert | Bedingung | Verwandte Standards |
---|---|---|---|
Dichte | 2,69 g/cm³ | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Mechanisch
Eigenschaft | Wert | Bedingung | Verwandte Standards | Kommentar |
---|---|---|---|---|
Elastizitätsmodul | 70,0 GPa | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 | |
Härte, Brinell | 62,0 [-] | O | AA-Standards | |
Plane-Strain-Bruchzähigkeit | 22,0 - 35,0 MPa·√m | Typisch für geschmiedetes Aluminium der Serie 5000 | ||
Poisson-Zahl | 0,33 [-] | Typisch für geschmiedetes Aluminium der Serie 5000 | ||
Schermodul | 26,0–26,5 GPa | Typisch für geschmiedetes Aluminium der Serie 5000 | ||
Zugfestigkeit | 215,0 - 285,0 MPa | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 | |
250,0 MPa | O | AA-Standards |
Thermisch
Eigenschaft | Temperatur | Wert | Bedingung | Verwandte Standards | Kommentar |
---|---|---|---|---|---|
Wärmeausdehnungskoeffizient | 20 °C | 2.36e-05 1/K | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 | |
100 °C | 2.36e-05 1/K | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 | ||
Max. Betriebstemperatur | 150,0 °C | Typisch für geschmiedetes Aluminium der Serie 5000 | |||
Schmelzpunkt | 600,0 - 645,0 °C | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 | ||
Spezifische Wärmekapazität | 879,0 - 963,0 J/(kg·K) | Typisch für geschmiedetes Aluminium der Serie 5000 | |||
Wärmeleitfähigkeit | 134 W/(m·K) | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Elektrik
Eigenschaft | Wert | Bedingung | Verwandte Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 20000000,0 S/m | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Elektrischer Widerstand | 5e-08 Ω·m | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Chemische Eigenschaften
Eigenschaft | Wert | Bedingung | Verwandte Standards |
---|---|---|---|
Chrom | 0,05 - 0,2 % | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Kupfer | 0,1 % | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Eisen | 0,40 % | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Magnesium | 2,4 - 3,0 % | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Mangan | 0,5 - 1,0 % | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Silizium | 0,25 % | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Titan | 0,2 % | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Zink | 0,25 % | O | AA-Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Technologische Eigenschaften
Eigenschaft | ||
---|---|---|
Löten | Allgemein:Löten ist nicht bekannt oder entwickelt
| |
Korrosionseigenschaften | Spannungsrisskorrosion:keine Schäden bei Betrieb und Labortests, allgemein:sehr gut, ohne Schutz in Industrie- oder Meerwasseratmosphäre
| |
Allgemeine Bearbeitbarkeit | Allgemein:schlecht (O, H32, H111), ausreichend (H34)
| |
Arbeitbarkeit | Allgemein (Zustand):gut (O), akzeptabel (H32, H34, H111)
|
Metall